U. S. Department of Commerce National Bureau of Standards RESEARCH PAPER RP826 Part of Journal of Research of the National Bureau of Standards, Volume 15, September 1935 MECHANICAL PROPERTIES OF COTTON YARNS « By Herbert F. Schiefer and Daniel H. Taft abstract The results of tests on three lots of cotton yarns are discussed. Two of the lots (80s and 10s) were spun in the experimental mill of the National Bureau of Standards. The 80s yarn was spun from 1%6-inch staple Peeler cotton with 20 different twists. The 10s yarn was spun from 1-inch staple Upland cotton with 12 different twists. Both yarns were spun with right-hand (Z) and with left-hand (S) twist. The third lot was 2/160s mercerized yarn spun from 1%-inch staple Sea Island cotton. This yarn was considered to be of high commerical quality. The breaking strength and elongation at rupture were determined by single- strand, multiple-strand, and skein tests. The variation in breaking strength, elongation at rupture, diameter, angle of twist, and irregularity of the 80s and 10s yarns with the amount of twist are shown. The average breaking strength per strand and the elongation by the multiple-strand test are less than those by the single-strand test and greater than those by the skein test. The data were studied statistically and an explanation is given of the differences which were obtained by the different test methods. Twelve cones of the commercial yarn were tested for breaking strength by the single-strand test. A statistical study of the data indicates significant differences in the average breaking strengths between the different cones. Some of the factors which affect the strength of a cotton yarn are discussed. The formulas tan 0=irDT and T=M -y/C where /3, D, T, M, and C are angle of twist, diameter, turns of twist per inch, twist multiplier, and count respectively, are derived by assuming that the exposed fibers are arranged as helices on a circular cylinder and that 2 yarns of different counts have the same density when their angles of twist are equal. It was found that the values for the angle of twist computed by these formulas were consistently greater than the observed values. The empirical formula 0=— - — — — t=> where T=M -yfC } appears to 1 — 0.4 -y C give results which are in good agreement with the observed values. CONTENTS Page I. Introduction 238 II. Samples 238 III. Test procedure 239 1 . Breaking strength and elongation at rupture 239 2. Diameter and angle of twist 240 3. Formulas 240 IV. Results 241 1. Bureau's 80s (67.2 typp) cotton yarn 241 2. Bureau's 10s (8.4 typp) cotton yarn 247 3. Commercial cotton yarn, 2/160s (2/134.4 typp) 248 V. Factors affecting the strength of a cotton yarn 250 VI. Relations between diameter, angle of twist, count, and twist 251 i The authors express their appreciation to A. A. Mercier, who initiated part of this work, and lo J. W. Porter, who assisted in spinning, for their assistance in this investigation oefore they left the National Bureau of Standards. 237 238 Journal of Research of the National Bureau of Standards [Vol. is I. INTRODUCTION A cotton yarn is a heterogeneous material. It consists of a large number of individual cotton fibers which are held together by twist. The fibers are not uniform in length, cross section, and strength. They are unequally distributed throughout the length of the yarn. The resulting yarn is irregular and contains hard and soft places, large and small cross sections, and strong and weak places. A study of the irregularity of cotton yarn has recently been made by Lee. 2 His study is based upon a statistical analysis of the varia- tions in the weight of specimens 6 inches long. The specimens were taken at the various stages during the yarn manufacturing process, from the card sliver to the spun yarn. His results are of great interest since they show the processes where the irregularity is increased or decreased and indicate the processes where improvement in yarn manufacture can be made. In the experimental study of cotton fabrics at the National Bureau of Standards during the past 5 years a large amount of data has been obtained which shows the effect of twist on the strength, elonga- tion, diameter, angle of twist, and irregularity of cotton yarns. These data are reported and discussed in this paper. The influence of these characteristics on the properties of fabrics wx>ven from these yarns will be reported in 2 subsequent papers. II. SAMPLES Two lots of the cotton yarn discussed in this paper were spun in the experimental cotton mill of the Bureau. The third lot of yarn was a commercial product. Information relative to the cotton and processing of the yarns spun at the Bureau is given in table 1. Table 1. — Manufacturing details of the cotton yarns spun at the Bureau Variety of cotton Grade Staple length, inch Breaker picker lap, oz/yd Intermediate picker lap, oz/yd Finisher picker lap, oz/yd Card sliver, grains/yd Sliver lap, grains/yd Ribbon lap, grains/yd Comber sliver, grains/yd First drawing sliver, grains/yd Second drawing sliver, grains/yd Finisher drawing sliver, grains/yd Slubber roving, hanks/lb a Intermediate roving, hanks/lb Second intermediate roving, hanks/lb _ Jack roving, hanks/lb Yarn, counts * Peeler Good middling- 1Mb 15 475.. 55. _ 52._. 50 0.50 1.26 4.04 15.29 80s (67.2 typp). Upland Good ordinary 1 18 17 16 64 59 53 0.53 1.26 2.10 10s (8.4 typp). » A hank of cotton roving is equal to 840 yards. * Count is the number of hanks per pound. " Typp " denotes the number of thousand yards per pound. The typp system provides a rational method of designating the size of all yarns, regardless of the kind of fiber composition. It was sponsored by E. D. Fowle in Textile World, 81, 1,470 (Apr. 23, 1932). The 80s yarn was spun with 20 different twists. The 10s yarn was spun with 12 different twists. The twist multipliers varied from 2.48 to 6.66 for the 80s yarn and from 2.25 to 9 for the 10s 2 R. L. Lee, Jr. A critical study of cotton manufacturing processes, Textile Research IV, no. 5, 235-260 (March 1934); V no. 4, 167-183 (February 1935); V, no. 7, 326-336 (May 1935). Ta}t fer ] Properties of Cotton Yarns 239 yarn. The number of turns of twist per inch, T, for each yarn may be calculated by using the formula T=M!+•- S--9 ■ 4--8 •I - 9 7 TWIST MULTIPLIER 6.11 COEF OF VAR. STRENGTH 23.5 % ELONGATION 14.7 % AVERAGE 13 12 l|Z UJ °z o 7§ z o _J 6 W 3 4 STRENGTH - 6 2 3 OUNCES Figure 1. — Scatter diagrams for three-twist multipliers of 80s cotton yarn. high elongation at rupture, carry a load less than their ultimate breaking strength when the load carried by the aggregate is a maxi- mum. The ratio of the average breaking strength per strand by the multiple-strand test to the average breaking strength per strand b} r the single-strand test is a fraction which decreases, in general, with an increase in twist multiplier. This decrease is readily explained by the variation in the irregularity of the yarn with respect to elongation at rupture, which is measured by the coefficient of variation and takes into consideration the variations of both the magnitude and the spread of the elongation at rupture with an increase in twist multiplier. It should be noted that the single-strand tests were made at a lower speed than the multiple-strand tests. This factor may have some effect on the results. Similar variations are also found for average elongation by the two methods of test, where elongation by the multiple-strand test refers Schieferl Tuft J Properties of Cotton Yarns 245 to the elongation corresponding to the maximum load carried by the 100 strands. In the regular skein test, 160 strands, 80 loops, are subjected to tension simultaneously. Each strand is in effect 27 inches long. On the basis of the discussion given above for the multiple-strand test the average breaking strength per strand and the elongation at the maxi- mum load carried by the skein are expected to be lower than those 3 — « — r -t 1 1 } i 1 r- ELONGATION DIAMETER AND ANGLE OF TWIST # DIAMETER TWIST MULT I PL I ERS • MULTIPLE STRAND SINGLE STRAND Figure 2. — Effect of tivist multiplier on the breaking strength, elongation at rapture, diameter, and angle of twist of the 80s cotton yarn. The differences in the results obtained by the three methods of determining the strength and elongation are also shown. obtained by the single-strand test. An additional reduction is to be expected because the variations occurring in specimens 27 inches long are greater than those found in specimens only 4 inches long. The ratio of the average breaking strength per strand by the skein test to the average breaking strength per strand by the single-strand or by the multiple-strand test is a fraction which decreases in general with an increase in twist multiplier. The results for strength and elongation by the three methods of test are plotted in figure 2 against twist multiplier. The graphs indi- cate the variation of strength and elongation with twist multiplier for 246 Journal of Research of the National Bureau of Standards [Vol. is each method of test as well as the relationship for strength and elonga- tion between the three methods of test. The maximum strength by 5- O 3 ^ bJ 2 I i I I I I I r I l . • ! 1 _• ml LLGi-'-'-J-i- «.' '...••!T.i. . * *• *! TWIST MULTIPLIER 2.5 COEF OF VAR. STRENGTH 19.7 % ELONGATION 25 % t i i i i i i i i i r I . ' I. ' .*! '*' ■ — - — rr T *nJ ,T ~~ — • AVERAGE I I I I I I I TWIST MULTIPLIER 3.75 3 . COEF OF VAR. STRENGTH aO % 2 . ELONGATION 6£ % I -f ~~ AVERAGE I +-- I TT 16 •15 •14 13 12 •II •10 •9 8 •7 * i . i i •i ...i *. i • ." i jiiiii -^-7—-- •*! * . " l TWIST MULTIPLIER 8 COEF OF VAR. STRENGTH 15.4 S ELONGATION 14.1 % I AVERAGE + I I ' I I I ' I I 'I ' I I 17 16 15 1 14! ( L 13 °- 12 O 10 < o z 90 U) 8 7 8 10 12 14 16 18 20 22 24 26 28 30 32 10 12 14 16 18 20 22 STRENGTH OUNCES Figure 3. — Scatter diagrams for three-twist multipliers of 10s cotton yarn. ELONGATION _1_ -J l_ _J i L_ ? 3 O SKEIN 7 TWIST MULTIPLIERS 4 * • MULTIPLE STRAND • SINGLE STRAND Figure 4. — Effect of twist multiplier on the breaking strength, elongation at rupture, diameter, and angle of twist of the 10s cotton yarn. The differences in the results obtained by the three methods of determining the strength and elongation are also shown. the multiple-strand and skein tests appears to occur at a slightly lower twist multiplier than for the single-strand test. This is in agreement Schiefer'] Taft J Properties of Cotton Yarns 247 with the shift noted by Mercier 6 for combed and carded cotton yarns. He reported maximum strength at twist multiplier 5.25 for the single- strand test and at 4.25 for the skein test of the same yarns. This shift can be explained on the basis of an increase in irregularity of the yarn with respect to elongation as the twist multiplier is increased. Unfortunately Mercier did not investigate this property in his study. The variations of diameter and angle of twist with twist multiplier are also shown in figure 2. The diameter decreases and the angle of twist increases with an increase in twist multiplier. 2. BUREAU'S 10s (8.4 TYPP) COTTON YARN There appeared to be no consistent difference in the data for yarns spun from single and from double roving with right-hand and with left-hand twist for the various twist multipliers. No distinction is therefore made in the results presented. The variations in breaking strength and in elongation at rupture by the single-strand test for the various twist multipliers are shown by frequency distributions in tables 4 and 5, respectively. The average, standard deviation, coefficient of variation, standard error of the Table 4. — Frequency distribution of breaking strength of 10s cotton yarn by the single-strand test Breaking strength (in oz) Twist multiplier at cell midpoint 2.25 2.5 3 3.5 3.75 4 4.5 4.75 6 7 8 9 4.5 5 14 34 26 15 6 5.5 6.5 7.5 8.5 4 9 5 9 15 9 20 10 6 9 2 2 1 9.5 6 10.5 1 4 6 18 19 18 6 9 9 1 5 4 19 11.5. 13 12.5 2 1 12 19 21 9 11 12 4 6 3 10 13.5 24 14.5 1 4 3 5 3 10 10 11 13 8 14 6 5 1 3 1 1 1 4 12 11 11 15 12 10 8 3 2 6 2 2 2 10 15.5 . 6 16.5 8 17.5 1 1 6 9 13 7 15 13 13 8 4 3 4 3 1 18.5 2 7 10 12 17 15 13 12 7 5 1 19.5 1 20.5 21.5 4 5 1 10 7 20 32 6 10 5 3 7 5 15 17 16 16 10 6 3 2 11 10 9 10 15 13 5 7 10 5 2 3 22.5 23.5 24.5 25.5 26.5 .. 27 5 28.5 29.5 30.5 31.5 32.5 Total 100 7.0 1.22 17. 4± 1.27 9.4=fc 1.40 6.7 100 13.6 2.68 19. 7± 1.45 11. 7± 1.56 7.5 100 17.3 2.30 13.4=b 0.97 5.4=b 1.13 4.8 100 23.2 2.26 9.7d= 0.69 1.7± 0.89 1.9 100 26.7 2.13 8.0=fc 0.57 0.0=b 0.81 100 26.2 2.26 8.6=b 0.62 0.6=L 0.84 0.7 100 25.9 3.04 11. 8± 0.85 3.8=L 1.02 3.7 100 24.9 2.93 11.8=1= 0.85 3.8=fc 1.02 3.7 100 22.2 3.50 15.8d= 1.15 7.8=h 1.28 6.1 100 19.3 3.08 16.0=fc 1.16 8.0=fc. 1.29 6.2 100 16.6 2.55 15.4=b 1.12 7.4± 1.26 5.9 100 Average, A, oz Standard devia- tion, oz 12.9 2.24 Coefofvar., V, %..{ A=F-8.0, % { Significance ratio, R. 17. 4± 1.27 9.4=b 1.40 6.4 •A. A. Mercier and C. W. Schoffstall, Effect of twist on cotton yarns. BS J. Research 1, 733 (1928) RP27. 248 Journal of Research of the National Bureau of Standards [Vot. n Table 5. — Frequency distribution of elongation of 10s cotton yarn by the single- strand test Elongation (in %) at Twist multiplier cell midpoint 2.25 2.5 3 3.5 3.75 4 4.5 4.75 6 7 8 9 4 75 6 30 48 14 2 5.25 1 8 23 35 31 2 5 75 1 14 20 41 12 12 6.25 6 75 2 6 16 49 17 9 1 1 5 9 33 36 15 1 7.25 20 23 27 18 9 1 9 10 31 23 20 3 3 1 4 11 31 16 23 10 3 1 1 8 4 6 11 6 11 3 17 8 11 3 5 2 7.75 8.25 875 9.25 - - 2 9 26 17 24 7 14 1 ______ 6 15 7 27 4 17 9 7 1 9.75 - 10.25 10 75 11.25 11.75 12.25 12.75 13 25 13 75 ... 1 14.25. 4 14.75 4 15.25 -- --- 12 15.75 6 16.25 - - --- 8 16.75 --- --- 3 17.25 --- --- 13 17.75 11 18.25 11 1K.75 2 19.25 7 19.75 5 20.25 3 20.75 _ 2 21.25 3 21.75 2 22.25 1 22.75 2 Total 100 5.63 0.42 J7.4_fc \0. 53 J0.9± \0.70 1.3 100 6.72 0.51 7.5_fc 0.54 1.0± 0.71 1.4 100 7.18 0.60 8.3± 0.59 1.8± 0.75 2.4 100 8.27 0.55 6.6_fc 0.47 0.1± 0.66 0.2 100 8.49 0.55 6.5db 0.46 O.Odb 0.65 100 9.07 0.65 7.2± 0.51 0.7± 0.69 1.0 100 9.51 0.73 7.7± 0.55 1.2db 0.72 1.7 100 9.69 0.79 8.2_fc 0.59 1.7± 0.75 2.3 100 10.92 0.81 7.4db 0.53 0.9± 0.70 1.3 100 12. 33 1.14 9.2=b 0.66 2.7± 0.80 3.4 100 13. 33 1.88 14.1_fc 1.02 7.6=fc 1.12 6.8 100 Average, A. % Standard devia- tion, % 17.76 2.09 Coefofvar., V,%— A=V-&.5,% Significance ratio, E. 11.8_b 0.85 5.3± 0.97 5.5 coefficient of variation, the difference between the minimum coeffi- cient of variation at twist multiplier 3.75 and the coefficient of varia- tion for the other twist multipliers, the standard error of these differ- ences, and the significance ratio of these differences are also given in the tables for the various twist multipliers. The scatter diagrams shown in figure 3 are for twist multipliers 2.5, 3.75, and 8. The results for strength and elongation by the three methods of tests are plotted in figure 4 against twist multiplier. The variations in diam- eter and angle of twist with twist multiplier are also shown in figure 4. In general, the same conclusions may be drawn from these results as were made for the 80s cotton yarns. They are not discussed indi- vidually for the sake of brevity. 3. COMMERCIAL COTTON YARN, 2/160s (2/134.4 TYPP) Forty pounds of 2/1 60s mercerized cotton yarn of high commercial quality were purchased for a study of cotton fabrics for parachutes. One hundred breaking-strength determinations were made by the Schieferl Taft J Properties of Cotton Yarns 249 single-strand test on each of 12 cones of yarn selected at random from the entire lot. The variations in brealung strength of the yarn from the different cones and from the entire lot are shown by frequency distributions in table 6. The average, standard error of the average, standard deviation, coefficient of variation, difference between average of cone no. 1 and average of the other cones, and the standard error and significance ratio of these differences are also given in table 6. Table 6. — Frequency distribution of breaking strength for 12 cones of 2jl60s mercerized cotton yarn of high commercial quality Breaking strength (in Cone numbers oz) at cell midpoint 1 2 3 4 5 6 7 8 9 10 11 12 1 to 12, inch 3.5.. 1 1 2 2 8 15 23 18 10 14 4 2 l 4.0 1 2 6 13 19 13 13 11 6 6 2 4.5 2 1 3 12 14 24 7 12 7 7 2 1 2 6 10 18 23 10 10 10 5 3 2 3 5.0 . . 1 2 9 15 17 20 18 3 6 6 2 1 3 1 4 7 17 22 15 11 10 9 1 1 1 6 7 7 23 6 28 12 7 I ..... 4 6 10 21 12 17 8 10 2 1 2 2 6 10 12 11 10 9 13 10 10 3 2 ..... 6 10 10 10 10 14 17 9 7 4 1 2 10 5.5... 6.0 6,5. _. 4 7 8 22 21 17 7 6 6 2 2 4 17 IS 22 9 9 7 8 1 2 23 72 123 7.0 7.5 181 237 8.0 137 8.5 9.0 . 147 111 9.5 . 84 10.0 41 10.5 21 11.0 4 11.5 3 Total Avernge, A,oi.. Standard devi- ation, oz Coef of var., V, % 100 /7. 24± \0. 108 1.07 14.8 /0. OOdb 10. 152 100 7.48dr 0.120 1.19 15. 9 0.24± 0.161 1.5 100 7.48± 0.120 1.19 15.9 0.24± 0.161 1.5 100 7.54± 0.104 1.03 13.7 0. 30± 0.149 2.0 100 7.66± 0.116 1. 15 15.0 0.42± 0.158 2.7 100 7. 694= 0.117 1.16 15.1 0. 45± 0. 158 2.9 100 7.73± 0.109 1.08 14.0 0. 49± 0.153 3.2 100 7. 9S 1 0.107 1.06 13.3 0. 74± 0. 151 4.9 100 8.02± 0.130 1.29 10.1 0.78± 0.168 4.7 100 8. 09 -i= 0. Ill 1.10 13.8 0. 85zh 0.154 5.5 100 8. 11± 0.144 1.43 17.6 0.87± 0.180 4.8 100 8.29± 0.135 1.34 16.2 1.05± 0. 172 6.1 1,200 7. 774± 0.122 1. 215 15.7 A=.4-7.24, oz. Significance ra- tio, R 0. 534. b 0. 163 3.3 The average breaking strength varies from 7.24 ounces for cone no. 1 to 8.29 ounces for cone no. 12. This variation is 13.5 percent of the average of 7.774 ounces for the entire lot and the difference between 7.24 and 8.29 ounces is 6.1 times its standard error, which is a significant difference. On the other hand the significance ratios of the differences between the average breaking strengths of cones nos. 1 and 12 and the average of the entire lot are 3.3 and 2.8, respectively. These values are close to the limiting value indicating a significance. The coefficient of variation, which is taken as a measure of irreg- ularity, varies from 13.3 to 17.6 percent between the different cones and is equal to 15.7 percent for the entire lot. This is somewhat higher than the irregularity of about 10 to 12 percent obtained for the 80s and 10s yarn for the twist multipliers yielding maximum strength. On the assumption that the single unmercerized yarn had the same irregularity as the Bureau's yarn it appears that plying and mercer- ization did not decrease the irregularity of this yarn materially. A more extensive study of the effect of these factors on the irregularity pf the yarn must be made, however, to establish this fact, 250 Journal of Research of the National Bureau of Standards \voi. u V. FACTORS AFFECTING THE STRENGTH OF A COTTON YARN The strength, length, and other characteristics of the cotton fibers have an effect on the strength of a cotton yarn. The relation of yarn strength to fiber strength has been discussed in considerable detail by Turner. 7 The strength of the yarn is related to the length of the cotton fiber. For example, it was found that a 10s yarn spun from the lKe-inch staple Peeler cotton had a breaking strength 63 percent greater than a 10s yarn spun with the same twist multiplier from the 1-inch staple Upland cotton. Similarly it is known that a combed yarn is stronger than a carded yarn spun from the same raw cotton because many of the shorter and inferior fibers are removed in the combing process. The effect of twist on the strength of the yarn is indicated inthis paper and confirms the results obtained in previous investigations. Imparting twist to a bundle of cotton fibers decreases the diameter of the bundle, that is, it brings the fibers in closer contact by a radial pressure, thereby increasing the frictional forces between fibers or the resistance of fiber slippage when tension is applied to the bundle. On the other hand twist introduces torsional forces or shearing stresses in the individual fibers thereby decreasing their breaking strength in tension. A moderate amount of twist reduces the diameter a con- siderable amount and therefore increases the frictional forces between the fibers, while it does not set up appreciable stresses in the fibers or produce an appreciable decrease in the breaking strength of the fibers in tension. 8 It is expected therefore that the strength of the yarn should increase very materially to a maximum with a moderate increase in twist. Additional increase in twist decreases the diam- eter slightly and the effects of the opposing strength factors balance each other approximately, producing relatively little change in the strength of the yarn from the maximum value. At high twist, how- ever, the increase in the friction between fibers due to an increase in twist or a decrease in diameter is negligible while the decrease in the fiber strength due to internal stresses becomes appreciable. The strength of the yarn decreases rapidly with an increase in high twist and for excessively high twist the yarn may break during the twisting process without the addition of any external tension. Two other factors are also operative in materially reducing the breaking strength of yarns at high twist relative to the breaking strength at low twist. They are (1) increase in the draft during spin- ning of yarns of high twist and (2) variation in twist between fibers near the axis and the surface of the yarn. Increasing the draft for high twist to keep the count of the yarn at no tension constant has the same effect as reducing the weight per unit length of the yarn when it is under a tension substantially equal to its breaking strength. The decrease is proportional to the difference in elongation at rupture between a low-twisted and a high- twisted yarn. The fibers located near the axis of the yarn are not twisted to the same degree as those near the surface. This difference increases » A. J. Turner, The foundation of yarn strength and yarn extension. J. Textile Inst. 19, T286-T314 (1928). 8 H. A. Hamm and E. S. Cleveland, Relation between the twist and certain properties of rayon yarns.. BS J. Research 7, 617 (1931) RP361. s T c a f fer ] Properties of Cotton Yarns 251 with twist. When tension is applied to yarn the fibers near the sur- face assume less of the load because of greater twist (greater elonga- tion) than the fibers near the axis. For higher and higher twist this difference increases and the fibers near the surface become less and less effective. The data in the literature seem to indicate that maximum strength of fine yarns is obtained at lower twdst multipliers than in coarse yarn. Furthermore, a yarn appears to increase in strength more rapidly than its weight, that is, a 20s yarn has in general a breaking strength more than twice as great as that of a 40s yarn. These observations may be explained as follows: A fine yarn is usually spun from longer staple fiber and the ratio of the circumference of the yarn to the area of its cross section is greater in fine yarns than in coarse yarns. The longer fibers require less twist to increase the resistance of fiber slippage and the fibers retain more of their initial strength because the internal stresses due to twist are still small. Because of the greater ratio of the circumference to the cross-sectional area a smaller percentage of the total number of fibers are completely imbedded in the yarn or a greater percentage are exposed at the sur- face. The increase in twist cannot increase the frictional resistance of the fibers exposed at the surface. Both of these factors tend to produce maximum strength at lower twist multipliers. They ex- plain why maximum strength is obtained at a lower twist multiplier in fine yarn than in coarse yarn. The second factor explains why a 20s yarn, for example, has a breaking strength equal to more than twice that of a 40s yarn spun from the same raw cotton. The cross-sectional area of the 20s yarn is twice that of the 40s yarn, while the circumference of the 20s yarn is only 1.414 times that of the 40s yarn. Because a greater percent- age of the total number of fibers are exposed on the surface in fine yarns and are therefore comparatively ineffective, it is apparent why the breaking strength increases at a greater rate than the rate of increase in weight, all other factors remaining constant. VI. RELATIONS BETWEEN DIAMETER, ANGLE OF TWIST, COUNT, AND TWIST A direct relationship between diameter and angle of twist with twist multiplier has been indicated for 2 counts in this paper. In fact the formula T=M^C, which has been used for many years and was presented by Joseph Kochlin on November 28, 1828, before the Societe Industrielle de Mulhouse, 9 expresses a simple relationship between the count, twist multiplier, and number of turns of twist per inch. This formula can be readily derived by assuming that the exposed fibers are arranged as helice3 on a circular cylinder and that 2 yarns of different count have the same density when their angles of twist are equal. The projection of a helix on the z?/-plane may be expressed by the equation y=D/2 sin 2tTx where the x-axis coincides with the axis of the cylinder, D is the diameter and T is the number of turns of twist per inch. The angle I H. Briiggemann, Zwirne, p. 103 (1933). Published by R. Oldenbourg, Munich and Berlin, Germany, 252 Journal oj Research oj the National Bureau oj Standards [Vot. ts of twist is by definition equal to the angle which a tangent line makes with the x-axis at the origin of the above curve. If is the angle of twist, then it follows by differentiation that dy/dx= t&n. p=irDT when x=0 Let D and T represent the diameter and number of turns of twist per inch of a yarn of count Cand D' and T f similar values of a yarn of count C . If these 2 yarns have the same angle of twist then T=TD'ID. If w represents the weight per unit length of yarn of count C, 8 the density, and k a constant, then k/C=w=TdlD 2 /4: and IclC'=w' = Tr8'lD ,2 /4, since the count is inversely proportional to the weight. It follows therefore that D'/D= Js/S'-C/C and T= T'/tJ~C' • jC on the assumption that 5 = 8' when /3=P'. The expression T j^C is ordinarily termed the twist multiplier M and represents the number of turns of twist per inch in a yarn of count unity, C"=i. It is interesting to note that in Kochlin's derivation the additional assump- tion is made that the coefficient of friction between fibers is the same in yarns of different count when the exposed fibers make the same angle of twist. Kochlin expressed the coefficient of friction as equal to the tangent of the angle of twist. This expression is analogous to the common way of expressing the coefficient of friction between two surfaces. This assumption is very interesting and probably applies to the surfaces of the exposed fibers. It is not necessary, however, in the derivation of the above formula. In A of figure 5 are plotted the observed values of the angle of twist for 10s, 80s, 10 100s, 11 and 120s 12 yarn against the values com- puted from the formula tan p=irDT in which D was taken equal to observed diameters and T, the number of turns of twist per inch, was computed by the formula T=M^C. It is seen that the com- puted values are consistently greater than the observed values and the difference appears to increase with the count of the yarn. This indicates that the assumptions made in the above formulas are not strictly fulfilled in spun yarns. From the data at hand it is not possible to determine which assumption is in error. In fact it would be very difficult to determine because the yarn is irregular in other properties and probably varies as much in helical arrangement of the fibers, form of the cross section, and density. On the basis of experimental data Wagner and Herzog 13 have derived the empirical formula tan 0=0.873 irDT. The computed values of /3 for 10s yarn by this formula are in excellent agreement with the observed values, io ii 12 These yarns were spun from the same cotton. 1 3 P. Heermann und A. Herzog, Mikroskopische und mechanisch-technische Textiluntersuchungen, p. 233, Dritte Auflage (1931). Published by Julius Springer, Berlin, Germany. Schiefen Taft J Properties of Cotton Yarns 253 but the agreement is not very good for yarns of higher counts (see B of fig. 5). The empirical formula „_ arc tan wDT appears to give results which are in good agreement with the observed values for the yarns. The computed and observed values are plotted 50 SO if) 1 1 1 1 1 1 1 1 1 • 10 S YARN H rr a o 80S » 7\ In B the angle of twist, /8, was computed by using the formula tan &= 0.873 wDT. arctan -wDT In the angle of twist, /3, was computed by using the formula /3 —• 1— 0.4 VC in C of figure 5. The scattering of the points is probably attributable to the variability in the yarn and to the uncertainty in the measure- ments. Washington, July